Code
ISO 10675: acceptance levels for radiographs of welds.
The international standard that decides whether an indication on a weld radiograph is acceptable, at one of three acceptance levels.
What it covers
ISO 10675 in plain terms.
ISO 10675 is the acceptance half of weld radiography. ISO 17636 makes a valid radiograph; ISO 10675 decides what the indications on it mean for the weld.
It works in three acceptance levels. Acceptance level 1 is the strictest and goes with ISO 5817 quality level B; acceptance level 2 goes with quality level C, and acceptance level 3 with quality level D. The design or the application standard chooses the quality level, and the acceptance level follows.
Each imperfection is named with its ISO 6520-1 reference number, so a crack, a pore, a slag inclusion or lack of fusion means the same thing on every report in every language.
Part 1 covers steel, nickel, and titanium. Part 2 covers aluminum, linked to the quality levels of ISO 10042.
- Full title
- Non-destructive testing of welds — Acceptance levels for radiographic testing
- Parts
- Part 1: steel, nickel, titanium, and their alloys · Part 2: aluminum and its alloys
- Issued by
- ISO, adopted in Europe as EN ISO 10675
- Acceptance levels
- 1, 2, and 3, from the strictest
- Linked to
- ISO 5817 quality levels B, C, and D (ISO 10042 for aluminum)
- Technique standard
- ISO 17636
- Imperfection names
- Reference numbers from ISO 6520-1
Who it's for
One record. Both sides of the job.
How inspection works
Methods under ISO 10675.
Who sets the procedure, who sets acceptance, and who may do the work, method by method.
| Method | Procedure | Acceptance | Certification |
|---|---|---|---|
| Radiographic (RT), film or digital | ISO 17636-1 or -2 | ISO 10675-1 or -2 at acceptance level 1, 2, or 3 | ISO 9712 RT Level II interpreter |
Acceptance criteria
How a weld passes or fails.
Each imperfection type has its own limit at each acceptance level. The level is set before interpretation starts.
- Cracks aren't acceptable at any level.
- Lack of fusion and lack of penetration are limited or not accepted, depending on the level.
- Porosity is judged by pore size and by the projected area of pores in a reference area.
- Elongated inclusions and slag are limited by width and length against thickness.
- Surface imperfections, like undercut and excess penetration, are judged on the radiograph where they're visible, and visually as well.
The report has to state the acceptance level used, because the same radiograph can pass at acceptance level 3 and fail at acceptance level 1.
A summary, not the code. Limits and exceptions are in the edition your job works to.
The report
What ISO 10675 reports have to carry.
The fields a Level III checks before signing. Miss one and the report comes back.
- Weld and component ID, material, and thickness
- ISO 5817 quality level and the ISO 10675 acceptance level applied
- Reference to the ISO 17636 technique record
- Each indication: ISO 6520-1 reference number, location, and size
- Accept or reject per indication and per weld
- Repair and re-radiography
- Interpreter name, ISO 9712 certification and date
Standards logic
Checked at capture, not after the report.
Where Weld Done holds a code's acceptance limits, each RT, VT, and UT indication is checked against them as it's entered. A rejected one shows the clause, the value, and the limit.
Standards logic →Where reports go wrong
The ISO 10675 mistakes that send a report back.
How the job's procedures come from your plan
The NDT reporting checklist: eight ways to get reports right the first time
No acceptance level stated.
Without it, a reader can't tell if a weld passed at the level the design asked for.
Imperfections named in local terms.
ISO 6520-1 numbers make the call checkable by any reviewer. Local names don't.
Steel limits on aluminum.
Aluminium welds are judged to Part 2, not Part 1.
Related codes
The codes around it.
Edition referenced: ISO 10675-1:2021 and ISO 10675-2:2021. All codes and standards
FAQ
Questions.
Every other answer is on the FAQ page.
What are ISO 10675 acceptance levels?
Three levels, 1 to 3, with level 1 the strictest. They match ISO 5817 quality levels B, C, and D, so the quality level in the design sets the acceptance level for the radiograph.
What's the difference between ISO 10675-1 and -2?
Part 1 covers steel, nickel, titanium, and their alloys. Part 2 covers aluminum and its alloys.
How does ISO 10675 relate to ISO 5817?
ISO 5817 sets quality levels for weld imperfections. ISO 10675 turns those quality levels into acceptance levels for what can be seen on a radiograph.

See your own report rebuilt.
Book a 30-minute demo on one of your real reports.
Not ready to talk? The calculator works out hours and costs back from your own numbers.